To determine % nickel in alloy steel by DMG extraction into chloroform at 465 nm.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To determine % nickel in alloy steel by DMG extraction into chloroform at 465 nm.

Theoretical Foundations

After dissolving steel in acid, nickel is selectively extracted as red Ni(DMG)2 into chloroform (465 nm, ε ≈ 1.7 × 10⁴), leaving iron and chromium in the aqueous phase. The extraction both separates and concentrates nickel, allowing determination of tenths of a percent Ni in steel.

Required Apparatus & Chemicals

Laboratory Apparatus

  • UV-Vis spectrophotometer
  • Separating funnels
  • Hot plate
  • Volumetric flasks
  • Pipettes
  • Cuvettes

Chemical Reagents

  • Alloy steel (1.000 g)
  • HCl/HNO3 for dissolution
  • Dimethylglyoxime (1% in ethanol)
  • Ammonia (1:1)
  • Bromine water
  • Chloroform
  • Ni standard

Step-by-Step Practical Procedure

  1. Dissolve 1.000 g steel in HCl/HNO3; dilute to 100 mL.
  2. Take the full 100 mL (or a measured aliquot) to a separating funnel.
  3. Add bromine water, then ammonia until ammoniacal.
  4. Add DMG; extract twice with 10 mL chloroform.
  5. Combine extracts; dilute to 50 mL with chloroform.
  6. Extract Ni standards identically; zero at 465 nm with CHCl3; read and calculate % Ni.

Observations & Expected Results

Red complex concentrates in the chloroform layer; aqueous iron stays behind; A465 linear with nickel.

Worked Stoichiometric Calculations

Problem: 1.000 g steel to 100 mL; the whole digest extracted to 50 mL CHCl3 gives A = 0.350 at 465 nm (ε = 1.70 × 10⁴, l = 1 cm). Find % Ni.

Working: c = 0.350/1.70 × 10⁴ = 2.06 × 10⁻⁵ mol L⁻¹. Mass in 0.050 L = 2.06 × 10⁻⁵ × 0.050 × 58.69 = 6.04 × 10⁻⁵ g. %Ni = 6.04 × 10⁻⁵/1.000 × 100 = 0.121%.

Safety Precautions & Hazard Control

  • Extract standards through the identical procedure to cancel extraction losses.
  • Vent the funnel when shaking chloroform.
  • Work in a fume cupboard with chloroform.
  • Keep the aqueous phase ammoniacal during extraction.

Waste Disposal Protocol

Chloroform layers to halogenated waste; acidic aqueous iron waste to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why extract the standards too?

A: Extraction is never 100% efficient; identical treatment of standards cancels the recovery factor.

Q: Why does iron not extract with DMG?

A: Fe does not form a neutral chloroform-soluble DMG chelate under these conditions; it stays in the ammoniacal aqueous phase.

Q: What is the advantage of extraction over direct colorimetry?

A: It separates nickel from the intensely coloured iron matrix and concentrates it into a small organic volume, boosting sensitivity.