CHEMVEN

Copper in Brass: Ammonia Complex Method

To determine % copper in brass by dissolving the alloy and measuring [Cu(NH3)4]²⁺ at 610 nm.

Level: UniversitySafety: Advanced lab onlyTime: 2 h
Aim of Experiment: To determine % copper in brass by dissolving the alloy and measuring [Cu(NH3)4]²⁺ at 610 nm.

Theoretical Foundations

Brass (Cu-Zn alloy) dissolves in nitric acid; zinc stays colourless in ammonia while copper forms the deep-blue tetraammine complex (610 nm). After dilution into the calibration range, absorbance gives copper mass and hence % Cu in the alloy (typically 60-70% for common brass).

Required Apparatus & Chemicals

Laboratory Apparatus

  • UV-Vis spectrophotometer
  • Volumetric flasks 250, 100 mL
  • Hot plate
  • Pipettes
  • Cuvettes
  • Fume cupboard

Chemical Reagents

  • Brass sample (0.0500 g)
  • Nitric acid (conc.)
  • CuSO4 standard (100 mg L⁻¹)
  • Concentrated ammonia

Step-by-Step Practical Procedure

  1. Dissolve 0.0500 g brass in 5 mL conc. HNO3 in a fume cupboard; dilute to 250 mL.
  2. Prepare Cu standards 0-8 mg L⁻¹ with 10 mL conc. NH3 per 100 mL.
  3. Dilute 10.00 mL of the brass solution to 100 mL with ammonia added.
  4. Zero at 610 nm with the ammonia blank.
  5. Read standards and sample.
  6. Calculate % Cu in the brass.

Observations & Expected Results

Brass solution turns deep blue in ammonia; zinc contributes no colour; calibration linear at 610 nm (slope ≈ 0.0663 A·L mg⁻¹).

Worked Stoichiometric Calculations

Problem: 0.0500 g brass to 250 mL; 10.00 mL diluted to 100 mL gives A = 0.820 (slope 0.0663 A·L mg⁻¹). Find % Cu.

Working: c(measured) = 0.820/0.0663 = 12.37 mg L⁻¹. Stock = 123.7 mg L⁻¹. In 0.250 L: 30.9 mg Cu. %Cu = 30.9/50.0 × 100 = 61.8%.

Safety Precautions & Hazard Control

  • Dissolve brass only in a fume cupboard (nitrogen dioxide fumes).
  • Dissolve completely; undissolved metal biases the result low.
  • Add the same ammonia volume to every flask.
  • Lead in some brasses precipitates as sulfate; filter if turbid.

Waste Disposal Protocol

Ammoniacal copper/zinc/nitrate waste to the aqueous heavy-metal waste bottle.

Viva Voce Oral Defense Questions & Answers

Q: Why does zinc not interfere?

A: Zn²⁺ forms a colourless ammine complex, so at 610 nm only the blue copper complex absorbs.

Q: Why dissolve in nitric acid rather than HCl?

A: Nitric acid oxidises and dissolves copper alloys cleanly; HCl alone cannot oxidise copper metal.

Q: How would you determine zinc in the same solution?

A: By a separate method, e.g. EDTA titration or dithizone spectrophotometry, since zinc is invisible at 610 nm.

← Back to Experiments Directory