Manganese in Steel: Periodate Oxidation Method

To determine manganese in steel by periodate oxidation to permanganate at 525 nm.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To determine manganese in steel by periodate oxidation to permanganate at 525 nm.

Theoretical Foundations

Sodium periodate oxidises Mn(II) to MnO4⁻ in hot nitric acid without a catalyst (λmax 525 nm, ε ≈ 2.3 × 10³). Phosphoric acid masks iron. The method is a standard steelworks analysis for 0.1-2% Mn, with absorbance proportional to manganese after identical oxidation of standards and samples.

Required Apparatus & Chemicals

Laboratory Apparatus

  • UV-Vis spectrophotometer
  • Hot plate
  • Volumetric flasks 100 mL
  • Beakers
  • Pipettes
  • Cuvettes

Chemical Reagents

  • Steel drillings (0.200 g)
  • Sodium periodate
  • Nitric acid (1:1)
  • Phosphoric acid
  • Mn standard (100 mg L⁻¹)

Step-by-Step Practical Procedure

  1. Dissolve 0.200 g steel in 20 mL 1:1 HNO3 with heating.
  2. Add 5 mL H3PO4 and 0.5 g NaIO4; boil 2 min.
  3. Cool and dilute to 100 mL.
  4. Oxidize Mn standards (0-2 mg L⁻¹) identically.
  5. Zero at 525 nm with the reagent blank; read absorbances.
  6. Calculate % Mn in the steel.

Observations & Expected Results

Purple permanganate develops on boiling; standards and sample treated identically give a linear calibration at 525 nm.

Worked Stoichiometric Calculations

Problem: 0.200 g steel diluted to 100 mL gives A = 0.450 at 525 nm (ε = 2.30 × 10³, l = 1 cm). Find % Mn.

Working: c = 0.450/2.30 × 10³ = 1.96 × 10⁻⁴ mol L⁻¹. Mass in 0.100 L = 1.96 × 10⁻⁴ × 0.100 × 54.94 = 1.07 × 10⁻³ g. %Mn = 1.07 × 10⁻³/0.200 × 100 = 0.538%.

Safety Precautions & Hazard Control

  • Dissolve steel completely; undissolved carbides trap manganese.
  • Boil with periodate long enough for full oxidation.
  • Treat standards through the identical oxidation procedure.
  • Avoid chloride; it consumes periodate.

Waste Disposal Protocol

Neutralize acidic waste, reduce permanganate with bisulfite, dispose via heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why oxidize the standards as well as the sample?

A: To cancel any incomplete oxidation or matrix effects; both experience identical chemistry, so the calibration is valid.

Q: Why is this a steelworks standard method?

A: It is fast, uses stable permanganate colour, and covers the 0.1-2% Mn range typical of carbon steels.

Q: What does phosphoric acid do here?

A: It forms colourless ferric phosphate, removing the yellow Fe(III) background at 525 nm.