CHEMVEN

Manganese Determination: Persulfate Oxidation to Permanganate

To determine manganese in steel by oxidizing Mn(II) to permanganate with ammonium persulfate and measuring at 525 nm.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To determine manganese in steel by oxidizing Mn(II) to permanganate with ammonium persulfate and measuring at 525 nm.

Theoretical Foundations

Mn(II) is oxidised by persulfate, catalysed by Ag⁺, to the intensely purple MnO4⁻ ion (λmax 525 nm, ε ≈ 2.3 × 10³ L mol⁻¹ cm⁻¹). Phosphoric acid masks Fe(III) as a colourless complex so it does not interfere. Absorbance of the resulting permanganate is proportional to the original manganese.

Required Apparatus & Chemicals

Laboratory Apparatus

  • UV-Vis spectrophotometer
  • Volumetric flasks 250 mL and 100 mL
  • Hot plate
  • Beakers
  • Pipettes
  • Cuvettes

Chemical Reagents

  • Ammonium persulfate (solid)
  • Silver nitrate solution (0.1 M)
  • Phosphoric acid (conc.)
  • Mn standard solution (50 mg L⁻¹)
  • Steel sample
  • Nitric acid for dissolution

Step-by-Step Practical Procedure

  1. Dissolve 0.500 g steel in dilute HNO3 and dilute to 250 mL.
  2. Prepare Mn standards 0-4 mg L⁻¹ in 100 mL flasks.
  3. Add 5 mL H3PO4, 2 mL AgNO3 and 1 g persulfate to each flask and the sample aliquot.
  4. Heat to boiling 2 min until the purple colour fully develops; cool.
  5. Dilute to mark, zero at 525 nm with a reagent blank.
  6. Read absorbances and determine Mn from the calibration curve.

Observations & Expected Results

Purple permanganate colour develops on heating; calibration linear at 525 nm; phosphoric acid keeps the solution free of yellow Fe(III) colour.

Worked Stoichiometric Calculations

Problem: 0.500 g steel dissolved to 250 mL gives A = 0.380 at 525 nm (ε = 2.30 × 10³, l = 1 cm). Calculate % Mn in the steel.

Working: c = 0.380/2.30 × 10³ = 1.65 × 10⁻⁴ mol L⁻¹. Mass Mn in 0.250 L = 1.65 × 10⁻⁴ × 0.250 × 54.94 = 2.27 × 10⁻³ g. %Mn = 2.27 × 10⁻³/0.500 × 100 = 0.454%.

Safety Precautions & Hazard Control

  • Boil long enough for complete oxidation; incomplete oxidation gives low results.
  • Cool before diluting to the mark (volume changes with temperature).
  • Do not overheat after colour develops; permanganate decomposes on prolonged boiling.
  • Keep chloride out; Ag⁺ precipitates AgCl and loses catalytic action.

Waste Disposal Protocol

Neutralize acidic permanganate waste, reduce with bisulfite, and dispose via the heavy-metal aqueous waste stream.

Viva Voce Oral Defense Questions & Answers

Q: What is the role of Ag⁺ in this method?

A: Ag⁺ catalyses the oxidation of Mn(II) to MnO4⁻ by persulfate, which is otherwise very slow.

Q: Why is phosphoric acid added?

A: It complexes Fe(III) as colourless [Fe(PO4)2]³⁻, preventing the yellow iron colour from interfering at 525 nm.

Q: Why must chloride be absent?

A: Chloride precipitates the Ag⁺ catalyst as AgCl and can also be oxidised, consuming persulfate.

← Back to Experiments Directory