CHEMVEN

Lead in Battery Paste as Lead Sulfate

Determine lead in lead-acid battery paste by precipitation as PbSO4.

Level: UniversitySafety: Advanced lab onlyTime: 3 h
Aim of Experiment: Determine lead in lead-acid battery paste by precipitation as PbSO4.

Theoretical Foundations

Battery paste (PbO, PbO2, PbSO4 mixture) is digested in acid; all lead is brought into solution as Pb2+ (PbO2 is reduced with H2O2 or hydroxylamine). Adding sulfate precipitates lead sulfate: Pb2+ + SO4 2- → PbSO4(s). PbSO4 is the stoichiometric weighing form after drying at 150 C (it decomposes on strong ignition). GF for lead = M_Pb/M_PbSO4 = 207.2/303.26 = 0.6832.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Fume cupboard
  • Sintered-glass crucible
  • Oven at 150 C
  • Desiccator
  • Lead PPE (gloves, no dust inhalation)

Chemical Reagents

  • Battery paste sample
  • Nitric acid, dilute
  • Hydrogen peroxide, 3%
  • Sulfuric acid, dilute (1 M)
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 1.0 g of paste (avoid inhaling dust; wear gloves).
  2. Digest with 15 mL dilute HNO3 plus 5 mL 3% H2O2 to reduce PbO2, warming gently.
  3. Dilute to 150 mL; filter off any insoluble residue.
  4. Heat to near boiling; add 10 mL 1 M H2SO4 slowly with stirring.
  5. Digest warm 30 minutes; filter through a weighed sintered-glass crucible.
  6. Wash with dilute H2SO4 then water; dry at 150 C to constant mass.
  7. Weigh PbSO4; calculate % Pb.

Observations & Expected Results

Dark paste dissolves to a colourless solution; white heavy PbSO4 precipitates, typically about 0.85 g from 1 g paste.

Worked Stoichiometric Calculations

Problem: 1.000 g of battery paste gave 0.8520 g PbSO4. Calculate % Pb. (GF_Pb = 0.6832)

Working: Mass Pb = 0.8520 × 0.6832 = 0.5821 g. % Pb = (0.5821/1.000) × 100 = 58.21%.

Safety Precautions & Hazard Control

  • Lead compounds are toxic: gloves, no dust inhalation, fume cupboard.
  • Reduce all PbO2 or it stays undissolved and is lost.
  • Dry at 150 C; PbSO4 decomposes if ignited strongly.

Waste Disposal Protocol

All lead residues and filtrates to dedicated lead waste; never down the drain.

Viva Voce Oral Defense Questions & Answers

Q: Why add H2O2 during digestion?

A: To reduce insoluble PbO2 to soluble Pb2+ so that all lead enters the solution for precipitation.

Q: Why not ignite PbSO4?

A: It decomposes at high temperature (losing SO3), so it is only dried at 150 C as the weighing form.

← Back to Experiments Directory