CHEMVEN

Zinc as Zinc Pyrophosphate

Determine zinc in an alloy by precipitation as ZnNH4PO4 and ignition to Zn2P2O7.

Level: UniversitySafety: Needs supervisionTime: 4 h
Aim of Experiment: Determine zinc in an alloy by precipitation as ZnNH4PO4 and ignition to Zn2P2O7.

Theoretical Foundations

Zinc is precipitated analogously to magnesium: Zn2+ + NH4+ + HPO4 2- → ZnNH4PO4(s) + H+. Ignition gives zinc pyrophosphate: 2ZnNH4PO4 → Zn2P2O7 + 2NH3 + H2O. The gravimetric factor for zinc is 2 × M_Zn/M_Zn2P2O7 = 130.76/304.71 = 0.4291. Copper and iron must be removed beforehand as they also form phosphates.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beaker
  • Hot plate
  • Ashless filter paper
  • Porcelain crucible
  • Muffle furnace
  • Desiccator

Chemical Reagents

  • Zinc alloy sample (Cu/Fe removed or absent)
  • Hydrochloric acid, dilute
  • Diammonium hydrogen phosphate solution, 10%
  • Ammonia solution, concentrated and dilute
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.5 g alloy; dissolve in 15 mL dilute HCl.
  2. Remove interfering ions (precipitate Cu with H2S or Fe with ammonia) and filter.
  3. Dilute the filtrate to 150 mL; add 15 mL 10% (NH4)2HPO4.
  4. Add concentrated ammonia with stirring to strong alkalinity; stand 4 hours.
  5. Filter through ashless paper; wash with dilute ammonia.
  6. Ignite at 900 C to constant mass; weigh Zn2P2O7 and calculate % Zn.

Observations & Expected Results

White crystalline precipitate; white Zn2P2O7, typically about 0.31 g from 0.5 g alloy.

Worked Stoichiometric Calculations

Problem: 0.5000 g of alloy gave 0.3120 g Zn2P2O7. Calculate % Zn. (GF_Zn = 0.4291)

Working: Mass Zn = 0.3120 × 0.4291 = 0.1339 g. % Zn = (0.1339/0.5000) × 100 = 26.78%.

Safety Precautions & Hazard Control

  • Remove Cu2+ and Fe3+ first; both give insoluble phosphates.
  • Stand long enough for complete crystallisation.
  • Ignite to constant mass at 900 C.

Waste Disposal Protocol

Ammoniacal phosphate filtrates to aqueous waste.

Viva Voce Oral Defense Questions & Answers

Q: Which ions interfere and why?

A: Cu2+, Fe3+, Al3+ and Ca2+ form sparingly soluble phosphates under the ammoniacal conditions and would be weighed as zinc.

Q: Compare this with the magnesium pyrophosphate method.

A: The chemistry is identical (MNH4PO4 → M2P2O7); only the gravimetric factor differs, showing how one procedure serves several analytes.

← Back to Experiments Directory