TGA of Magnesium Carbonate: Carbonate Decomposition

Determine the decomposition temperature range and mass loss of MgCO3 → MgO.

Level: UniversitySafety: SafeTime: 2 h
Aim of Experiment: Determine the decomposition temperature range and mass loss of MgCO3 → MgO.

Theoretical Foundations

Magnesium carbonate decomposes: MgCO3 → MgO + CO2↑. The theoretical loss is 44.01/84.31 = 52.20%. Unlike CaCO3, MgCO3 decomposes at a moderate temperature (~350-500 C), so the step is easily followed in a furnace. The residue mass gives the MgO content, convertible to % Mg.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • Porcelain crucible (weighed)
  • Muffle furnace
  • Desiccator
  • Tongs

Chemical Reagents

  • Magnesium carbonate, pure (basic carbonate of known composition — use the normal carbonate)
  • Silica gel desiccant (for desiccator)
  • Distilled water (glassware rinsing)

Step-by-Step Practical Procedure

  1. Weigh accurately 1.500 g MgCO3 into a weighed crucible.
  2. Heat at 300 C for 30 minutes; cool and weigh.
  3. Heat at 500 C for 1 hour; cool and weigh.
  4. Reheat at 500 C to confirm constant mass.
  5. Calculate % loss and compare with 52.20% theoretical.

Observations & Expected Results

White powder throughout; mass stabilises after the 500 C step.

Worked Stoichiometric Calculations

Problem: 1.500 g MgCO3 (M = 84.31) decomposed fully. Calculate the theoretical MgO residue (M = 40.30) and % loss.

Working: MgO = 1.500 × 40.30/84.31 = 0.717 g. Loss = 1.500 − 0.717 = 0.783 g → 52.20%, matching the theoretical CO2 loss.

Safety Precautions & Hazard Control

  • Confirm constant mass; basic carbonates decompose over a range.
  • Vent CO2; ensure furnace ventilation.
  • Use the normal carbonate of known stoichiometry for clean results.

Waste Disposal Protocol

MgO residue to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why does MgCO3 decompose at a lower temperature than CaCO3?

A: The small, highly polarising Mg2+ ion distorts the carbonate ion more strongly (Fajan's rules), destabilising it toward CO2 loss.

Q: What does the single sharp step tell you?

A: That decomposition goes directly to MgO with no stable intermediate — a clean one-step TGA curve.

← Back to Experiments Directory