Zinc by Electrogravimetry from Alkaline Bath
Determine zinc in an alloy by electrodeposition from alkaline zincate solution.
Theoretical Foundations
Zinc deposits from alkaline solution as the metal: [Zn(OH)4]2- + 2e- → Zn(s) + 4OH-. Alkaline conditions prevent hydrogen interference and keep aluminium (common alloy partner) dissolved as aluminate. The cathode gain is zinc directly. Copper, if present, must be removed first since it deposits preferentially.
Required Apparatus & Chemicals
Laboratory Apparatus
- Analytical balance
- Platinum or nickel cathode (weighed)
- DC power supply
- 250 mL beaker
- Oven
- Desiccator
Chemical Reagents
- Zinc alloy sample (Cu-free)
- Sodium hydroxide solution, 2 M
- Distilled water
- Ethanol
Step-by-Step Practical Procedure
- Weigh the cathode.
- Weigh 0.4 g alloy; dissolve in dilute HCl, then make strongly alkaline with 2 M NaOH.
- Filter off any precipitated impurities (e.g. Fe(OH)3).
- Electrolyse the clear zincate solution at 2 A for 45 minutes with stirring.
- Test completeness; wash with current on; rinse with ethanol and dry at 110 C.
- Weigh; the gain is zinc; calculate % Zn.
Observations & Expected Results
Grey adherent zinc deposit; typical gain about 0.097 g from 0.4 g alloy.
Worked Stoichiometric Calculations
Problem: 0.4000 g of alloy gave a cathode gain of 0.0965 g Zn. Calculate % Zn.
Working: % Zn = (0.0965/0.4000) × 100 = 24.13%.
Safety Precautions & Hazard Control
- Remove copper first if present; it codeposits with zinc.
- Keep the bath strongly alkaline or Zn(OH)2 precipitates.
- Zinc deposits oxidise in air; weigh promptly after drying.
Waste Disposal Protocol
Alkaline zinc electrolytes neutralised; residues to heavy-metal waste.
Viva Voce Oral Defense Questions & Answers
Q: Why deposit zinc from alkaline rather than acid solution?
A: In acid, hydrogen evolves preferentially on zinc (high overpotential issues and redissolution); alkaline zincate gives smooth, adherent deposits with good efficiency.
Q: What happens to aluminium in this bath?
A: It stays dissolved as aluminate [Al(OH)4]-, which needs a far more negative potential to reduce, so it does not contaminate the zinc deposit.