Electrogravimetric Determination of Copper in Brass
Determine copper in brass by electrodeposition on a weighed platinum cathode.
Theoretical Foundations
In electrogravimetry the analyte is deposited by electrolysis and weighed on the electrode: Cu2+ + 2e- → Cu(s). Brass is dissolved in HNO3; at controlled current copper deposits quantitatively on the Pt gauze cathode while zinc stays in solution (its deposition potential is much more negative). The mass gain of the cathode is the mass of copper directly — no gravimetric factor is needed.
Required Apparatus & Chemicals
Laboratory Apparatus
- Analytical balance
- Platinum gauze cathode and anode (weighed cathode)
- DC power supply with ammeter
- 250 mL beaker
- Hot plate
- Fume cupboard
- Oven
- Desiccator
Chemical Reagents
- Brass sample
- Nitric acid, dilute (1+1)
- Sulfuric acid, dilute
- Distilled water
- Ethanol (rinsing)
Step-by-Step Practical Procedure
- Weigh the clean Pt cathode accurately (mass A).
- Weigh 0.5 g brass; dissolve in 15 mL dilute HNO3 in a fume cupboard.
- Evaporate with 5 mL dilute H2SO4 to remove nitrate; dilute to 150 mL.
- Immerse the electrodes; electrolyse at 2 A with stirring for 45 minutes.
- Test completeness: expose a fresh cathode surface (raise the level) — no new deposit should form.
- Without switching off, wash the cathode with water, then ethanol; dry at 110 C.
- Cool in a desiccator and weigh (mass B); Cu = B − A.
- Calculate % Cu.
Observations & Expected Results
Pink copper coats the cathode; the blue solution fades to colourless. Typical deposit about 0.34 g from 0.5 g brass.
Worked Stoichiometric Calculations
Problem: Cathode 15.0000 g; cathode + deposit 15.3425 g, from 0.5000 g brass. Calculate % Cu.
Working: Mass Cu = 15.3425 − 15.0000 = 0.3425 g. % Cu = (0.3425/0.5000) × 100 = 68.5%.
Safety Precautions & Hazard Control
- Never switch off before washing: the deposit redissolves in the acidic bath without current.
- Remove nitrate by fuming with H2SO4 or deposition is incomplete.
- Wash the cathode thoroughly while the current is still on.
Waste Disposal Protocol
Acidic zinc-containing electrolyte to heavy-metal waste.
Viva Voce Oral Defense Questions & Answers
Q: Why must the current stay on during washing?
A: Without cathodic protection the acidic electrolyte chemically attacks the copper deposit, redissolving part of it and giving low results.
Q: Why doesn't zinc deposit with the copper?
A: Zn2+/Zn has a far more negative reduction potential (−0.76 V vs +0.34 V for Cu2+/Cu), so at the controlled conditions only copper reduces.
Q: Why is no gravimetric factor needed?
A: The weighed deposit is the pure analyte metal itself, so its mass is the copper mass directly.