CHEMVEN

Ash Content of Coal

Determine the ash content of coal by ignition at 815 C.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine the ash content of coal by ignition at 815 C.

Theoretical Foundations

Ash is the incombustible mineral residue (clay, quartz, pyrite products) left after burning coal: % ash = (residue/sample) × 100. Standard ashing at 815 C burns carbon fully while limiting decomposition of carbonates and oxidation artefacts. Ash content directly reduces calorific value and indicates slagging tendency.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • Weighed silica crucible
  • Muffle furnace at 815 C
  • Desiccator
  • Tongs

Chemical Reagents

  • Coal sample, ground to <212 µm
  • Silica gel desiccant (for desiccator)
  • Distilled water (glassware rinsing)

Step-by-Step Practical Procedure

  1. Weigh a silica crucible (mass A); add about 2 g of ground coal; weigh (mass B).
  2. Heat gently with the lid ajar to drive off volatiles without flaming.
  3. Ignite at 815 C for 1 hour.
  4. Cool in a desiccator and weigh (mass C).
  5. Re-ignite 15 minutes to confirm constant mass.
  6. Calculate % ash = (C − A)/(B − A) × 100.

Observations & Expected Results

Coal burns with brief flaming, leaving a pale grey ash, typically about 0.19 g from 2 g coal.

Worked Stoichiometric Calculations

Problem: Crucible 20.0000 g; crucible + coal 22.0000 g; crucible + ash 20.1860 g. Calculate % ash.

Working: Ash = 0.1860 g from 2.0000 g. % ash = (0.1860/2.0000) × 100 = 9.30%.

Safety Precautions & Hazard Control

  • Heat gently at first; violent volatile release can eject particles.
  • Use the standard 815 C; higher temperatures decompose carbonates and change the ash mass.
  • Cool fully in a desiccator; ash is hygroscopic.

Waste Disposal Protocol

Coal ash to solid waste.

Viva Voce Oral Defense Questions & Answers

Q: Why ash at 815 C specifically?

A: It is the ISO standard temperature: high enough to burn all carbon, low enough to avoid excessive carbonate decomposition and pyrite oxidation artefacts, keeping results comparable worldwide.

Q: How does ash affect coal use?

A: Ash is dead weight that lowers calorific value, causes slagging and fouling in furnaces, and must be disposed of.