Silicon in Ferrosilicon Alloy
Determine silicon in a ferrosilicon alloy by silica gravimetry.
Theoretical Foundations
Ferrosilicon is dissolved in a mixture of HNO3 and HF (silicon needs fluoride to dissolve): the silicon ends as H2SiF6. Fuming with H2SO4 expels fluoride, and evaporation with HCl dehydrates silicic acid to SiO2, which is filtered, ignited and weighed. The gravimetric factor for silicon is M_Si/M_SiO2 = 28.085/60.08 = 0.4674.
Required Apparatus & Chemicals
Laboratory Apparatus
- Analytical balance
- PTFE beaker
- Hot plate
- Ashless filter paper
- Platinum crucible
- Muffle furnace
- Desiccator
- HF handling kit
Chemical Reagents
- Ferrosilicon alloy, finely ground
- Nitric acid, concentrated
- Hydrofluoric acid
- Sulfuric acid, concentrated
- Hydrochloric acid, concentrated
- Distilled water
Step-by-Step Practical Procedure
- Weigh accurately 0.5 g of finely ground alloy into a PTFE beaker.
- In a fume cupboard add 10 mL conc. HNO3 and 5 mL HF; warm gently until dissolved.
- Add 10 mL conc. H2SO4; fume strongly to expel HF.
- Cool, add 20 mL conc. HCl and evaporate to dehydrate silica; bake at 110 C.
- Take up with HCl, filter the SiO2, wash.
- Ignite at 1000 C to constant mass; weigh SiO2 and calculate % Si.
Observations & Expected Results
Alloy dissolves with effervescence; white SiO2 residue, typically about 0.36 g from 0.5 g alloy.
Worked Stoichiometric Calculations
Problem: 0.5000 g of ferrosilicon gave 0.3580 g SiO2. Calculate % Si. (GF_Si = 0.4674)
Working: Mass Si = 0.3580 × 0.4674 = 0.1673 g. % Si = (0.1673/0.5000) × 100 = 33.47%.
Safety Precautions & Hazard Control
- HF and fuming H2SO4: advanced-lab PPE, fume cupboard, calcium gluconate gel.
- Use PTFE, never glass, while HF is present.
- Fume off ALL fluoride before filtering in glassware.
Waste Disposal Protocol
Fluoride waste to dedicated containers.
Viva Voce Oral Defense Questions & Answers
Q: Why is HF needed to dissolve ferrosilicon?
A: Silicon forms a protective SiO2 layer inert to ordinary acids; fluoride complexes it as soluble H2SiF6, breaking the passivation.
Q: Why fume with H2SO4 before the silica determination?
A: To expel all fluoride as HF/SiF4; residual fluoride would keep silicon in solution as fluorosilicate and give low results.