CHEMVEN

Silica in Portland Cement by Dehydration

Determine SiO2 in Portland cement by double dehydration of silicic acid.

Level: UniversitySafety: Needs supervisionTime: 4 h
Aim of Experiment: Determine SiO2 in Portland cement by double dehydration of silicic acid.

Theoretical Foundations

Acid decomposition of cement gives gelatinous silicic acid: SiO3 2- + 2H+ → H2SiO3. Evaporating to dryness and baking dehydrates it: H2SiO3 → SiO2 + H2O. Silica is filtered off, ignited and weighed directly — no gravimetric factor is needed since the weighing form is the analyte oxide. A second dehydration recovers the few percent of silica that escapes the first. Typical cement is ~20% SiO2.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Oven at 110 C and muffle furnace
  • Ashless filter paper
  • Platinum crucible
  • Desiccator
  • Hydrofluoric acid handling kit

Chemical Reagents

  • Portland cement sample
  • Hydrochloric acid, concentrated
  • Hydrofluoric acid (for impurity correction)
  • Sulfuric acid, dilute
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 1.0 g cement into a beaker.
  2. Add 15 mL conc. HCl; warm until decomposed.
  3. Evaporate to dryness on a hot plate; bake 1 hour at 110 C.
  4. Moisten with conc. HCl, add 50 mL hot water, digest and filter through ashless paper.
  5. Evaporate the filtrate again to dryness, bake and filter (second dehydration); combine precipitates.
  6. Ignite the combined silica at 1000 C to constant mass; weigh.
  7. Treat with HF + H2SO4, evaporate, reignite and reweigh; the mass loss is true SiO2.
  8. Calculate % SiO2.

Observations & Expected Results

Gelatinous silica on the filter; white ignited SiO2, typically about 0.21 g from 1 g cement.

Worked Stoichiometric Calculations

Problem: 1.000 g of cement gave 0.2135 g of HF-volatile SiO2. Calculate % SiO2.

Working: % SiO2 = (0.2135/1.000) × 100 = 21.35%, a normal Portland cement value.

Safety Precautions & Hazard Control

  • Bake the dehydration fully; incomplete baking leaves soluble silica.
  • HF is extremely hazardous: full PPE, fume cupboard and calcium gluconate gel available.
  • Ignite to constant mass; silica adsorbs water strongly.

Waste Disposal Protocol

HF-containing residues to dedicated fluoride waste; never mix with glass containers.

Viva Voce Oral Defense Questions & Answers

Q: Why dehydrate twice?

A: A few percent of silicic acid stays colloidal through the first filtration; the second evaporation recovers it, ensuring quantitative recovery.

Q: What is the HF treatment for?

A: HF volatilises SiO2 as SiF4; non-volatile impurities (Al2O3, Fe2O3) remain, so the mass loss gives true SiO2 free of contaminants.

← Back to Experiments Directory