CHEMVEN

Calcium in Dolomite by Oxalate (Monohydrate Weighing Form)

Determine calcium in dolomite, weighing the oxalate as CaC2O4·H2O.

Level: UniversitySafety: SafeTime: 3 h
Aim of Experiment: Determine calcium in dolomite, weighing the oxalate as CaC2O4·H2O.

Theoretical Foundations

Dolomite CaMg(CO3)2 dissolves in HCl. At pH ~4-5 calcium precipitates selectively as CaC2O4·H2O while magnesium stays in solution (see experiment 055). Drying at 105 C gives the stoichiometric monohydrate weighing form (GF = 0.2743), avoiding the 1000 C ignition and the hygroscopic CaO weighing.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beaker
  • Hot plate
  • Sintered-glass crucible
  • Oven at 105 C
  • Desiccator

Chemical Reagents

  • Dolomite sample, ground
  • Hydrochloric acid, dilute
  • Ammonium oxalate solution, 4%
  • Ammonia solution, dilute
  • Methyl red indicator
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.6 g dolomite; dissolve in 15 mL dilute HCl.
  2. Boil off CO2; dilute to 200 mL and heat.
  3. Add methyl red; precipitate with hot ammonium oxalate added slowly.
  4. Adjust to the yellow endpoint with ammonia; digest 1 hour.
  5. Filter through a weighed sintered-glass crucible; wash with cold water.
  6. Dry at 105 C to constant mass; weigh CaC2O4·H2O and calculate % Ca.

Observations & Expected Results

White precipitate; typical mass about 0.48 g from 0.6 g dolomite.

Worked Stoichiometric Calculations

Problem: 0.6000 g of dolomite gave 0.4755 g CaC2O4·H2O. Calculate % Ca.

Working: Mass Ca = 0.4755 × 0.2743 = 0.1304 g. % Ca = (0.1304/0.6000) × 100 = 21.74%, the theoretical value for pure dolomite.

Safety Precautions & Hazard Control

  • Control pH carefully to exclude magnesium.
  • Dry at 105 C, not higher.
  • Wash with cold water to minimise solubility loss.

Waste Disposal Protocol

Acidic filtrates neutralised.

Viva Voce Oral Defense Questions & Answers

Q: Why is the monohydrate form convenient here?

A: It needs only an oven, gives a large precipitate mass for precision, and avoids weighing hygroscopic CaO.

Q: How would you then determine magnesium in the same sample?

A: From the oxalate filtrate: precipitate MgNH4PO4 with phosphate and ammonia, ignite to Mg2P2O7 (see experiment 061).

← Back to Experiments Directory