Iron in Red Soil

Determine total iron in a red tropical soil by hydroxide gravimetry.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine total iron in a red tropical soil by hydroxide gravimetry.

Theoretical Foundations

Red soils are coloured by iron oxides (hematite, goethite). Acid digestion dissolves the iron; aluminium, also present, is kept in solution by precipitating iron selectively... in practice both precipitate, so iron is determined on the ignited mixed oxides only when Al is low, or Al is masked. Here the soil's iron is precipitated as Fe(OH)3 with ammonia and ignited to Fe2O3 (GF = 0.6994); aluminium interference is minimised by a single reprecipitation.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Ashless filter paper
  • Porcelain crucible
  • Muffle furnace
  • Desiccator

Chemical Reagents

  • Red soil, ground and sieved
  • Hydrochloric acid, concentrated
  • Nitric acid, concentrated
  • Ammonia solution, dilute
  • Ammonium chloride, solid
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 1.0 g of ground soil.
  2. Digest with 20 mL conc. HCl on a hot plate for 30 minutes.
  3. Dilute to 150 mL; filter off insoluble silica residue.
  4. Add NH4Cl, heat, precipitate with dilute ammonia; filter.
  5. Redissolve the precipitate in hot dilute HCl and reprecipitate with ammonia (double precipitation).
  6. Filter, wash, ignite at 850 C to constant mass; weigh Fe2O3 and calculate % Fe.

Observations & Expected Results

Reddish soil gives a yellow solution; brown Fe(OH)3 precipitate; reddish Fe2O3 after ignition, typically about 0.10 g.

Worked Stoichiometric Calculations

Problem: 1.000 g of red soil gave 0.0985 g Fe2O3. Calculate % Fe in the soil.

Working: Mass Fe = 0.0985 × 0.6994 = 0.06889 g. % Fe = (0.06889/1.000) × 100 = 6.89%.

Safety Precautions & Hazard Control

  • Digest long enough to dissolve iron oxide coatings.
  • Double-precipitate to separate iron from coprecipitated aluminium.
  • Filter off silica before precipitation.

Waste Disposal Protocol

Acidic soil digests neutralised before disposal.

Viva Voce Oral Defense Questions & Answers

Q: What gives red soils their colour?

A: Iron(III) oxides, mainly hematite (Fe2O3) and goethite (FeOOH), coating the soil particles.

Q: Why double-precipitate here?

A: Aluminium coprecipitates with Fe(OH)3; redissolving and reprecipitating leaves most aluminium in solution, giving a purer iron result.