CHEMVEN

Nickel in Bronze: Minor-Constituent Analysis

Determine a few percent nickel in a bronze alloy by DMG gravimetry.

Level: UniversitySafety: Advanced lab onlyTime: 3 h
Aim of Experiment: Determine a few percent nickel in a bronze alloy by DMG gravimetry.

Theoretical Foundations

Bronze is mainly copper and tin with minor nickel. After dissolution in acid, tin is removed as metastannic acid by evaporation with HNO3, and copper is held as the soluble ammine complex. Nickel is precipitated selectively: Ni2+ + 2 H2DMG → Ni(HDMG)2(s) + 2H+, GF = 0.2032. A larger sample (0.8 g) gives a weighable precipitate for a minor constituent.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 250 mL beaker
  • Hot plate
  • Fume cupboard
  • Quantitative filter paper
  • Sintered-glass crucible
  • Oven
  • Desiccator

Chemical Reagents

  • Bronze sample
  • Nitric acid, concentrated and dilute
  • Dimethylglyoxime solution, 1% in ethanol
  • Ammonia solution, dilute
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.8 g of bronze.
  2. Dissolve in 15 mL conc. HNO3 in a fume cupboard; evaporate to dryness to precipitate metastannic acid.
  3. Take up in dilute HNO3, filter off tin residue and wash.
  4. Dilute the filtrate to 150 mL; add DMG at 70-80 C, then ammonia to pH 8-9.
  5. Digest, filter through a weighed sintered-glass crucible, wash and dry at 150 C to constant mass.
  6. Weigh Ni(DMG)2 and calculate % Ni.

Observations & Expected Results

White metastannic acid residue filtered off; blue filtrate gives a small scarlet precipitate, typically about 0.12 g.

Worked Stoichiometric Calculations

Problem: 0.8000 g of bronze gave 0.1180 g Ni(DMG)2. Calculate % Ni.

Working: Mass Ni = 0.1180 × 0.2032 = 0.02398 g. % Ni = (0.02398/0.8000) × 100 = 3.00%.

Safety Precautions & Hazard Control

  • Remove tin fully; metastannic acid adsorbs nickel.
  • Fume cupboard for nitric acid dissolution.
  • Keep copper as the ammine with enough ammonia.

Waste Disposal Protocol

Acidic metal residues to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is tin removed as metastannic acid?

A: Tin(IV) hydrolyses to insoluble metastannic acid on evaporation with HNO3; if left, it would contaminate the nickel precipitate and adsorb nickel ions.

Q: Why use a larger sample for a minor constituent?

A: To bring the absolute mass of the precipitate into the accurately weighable range (ideally 0.1-0.5 g).

← Back to Experiments Directory