Nickel in Stainless Steel as Nickel Dimethylglyoximate

Determine nickel in steel by precipitation with dimethylglyoxime and weighing as Ni(DMG)2.

Level: UniversitySafety: Needs supervisionTime: 3 h
Aim of Experiment: Determine nickel in steel by precipitation with dimethylglyoxime and weighing as Ni(DMG)2.

Theoretical Foundations

Dimethylglyoxime (H2DMG) is a selective precipitant for Ni2+ in ammoniacal solution: Ni2+ + 2 H2DMG → Ni(HDMG)2(s) + 2H+. The scarlet-red chelate is very insoluble, stable to 150 C and highly selective — few ions interfere. Steel is first dissolved in acid and iron is kept in solution with tartaric acid (or removed) so it does not precipitate. The gravimetric factor is M_Ni/M_Ni(DMG)2 = 58.69/288.91 = 0.2032.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beakers
  • Hot plate
  • Sintered-glass crucible
  • Oven at 150 C
  • Desiccator
  • pH paper

Chemical Reagents

  • Steel sample (drillings)
  • Hydrochloric acid, dilute
  • Nitric acid, dilute
  • Tartaric acid solution, 10%
  • Dimethylglyoxime solution, 1% in ethanol
  • Ammonia solution, dilute (1+1)
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.4-0.5 g of steel drillings.
  2. Dissolve in 20 mL dilute HCl with a few drops of HNO3 on a hot plate; evaporate to low volume.
  3. Dilute to 200 mL, add 10 mL 10% tartaric acid to complex iron.
  4. Heat to 70-80 C and add 1% alcoholic DMG solution (about 30 mL) with stirring.
  5. Add dilute ammonia dropwise until just alkaline to litmus (pH 8-9); a scarlet precipitate forms.
  6. Digest warm 30 minutes; filter through a weighed sintered-glass crucible.
  7. Wash with hot water, dry at 150 C to constant mass, cool and weigh Ni(DMG)2.

Observations & Expected Results

Scarlet-red voluminous precipitate forms on adding ammonia. Typical mass 0.3-0.7 g from 0.5 g steel.

Worked Stoichiometric Calculations

Problem: 0.5000 g of steel gave 0.6120 g Ni(DMG)2. Calculate % Ni. (GF_Ni = 0.2032)

Working: Mass Ni = 0.6120 × 0.2032 = 0.1244 g. % Ni = (0.1244/0.5000) × 100 = 24.87%.

Safety Precautions & Hazard Control

  • Keep iron complexed with tartrate or it precipitates as hydroxide in ammonia.
  • Add ammonia slowly with stirring to avoid local excess and coprecipitation.
  • Dry at 150 C, not higher; the chelate decomposes above about 200 C.

Waste Disposal Protocol

Ethanolic DMG filtrates go to organic waste; nickel residues to heavy-metal waste.

Viva Voce Oral Defense Questions & Answers

Q: Why is dimethylglyoxime selective for nickel?

A: Ni2+ forms an exceptionally stable square-planar chelate with strong intramolecular hydrogen bonding, making Ni(HDMG)2 far less soluble than the complexes of most other metals.

Q: What is the role of tartaric acid?

A: It complexes Fe3+ (and Al3+) keeping them in solution when ammonia is added, so they do not precipitate as hydroxides with the nickel chelate.

Q: Why dry at 150 C rather than ignite?

A: Ni(DMG)2 is already a stoichiometric weighing form; ignition would decompose it to non-stoichiometric NiO.