Chloride in Rock Salt Ore: Grade Estimation

Estimate the NaCl grade of a rock-salt ore sample via chloride gravimetry.

Level: UniversitySafety: SafeTime: 2 h
Aim of Experiment: Estimate the NaCl grade of a rock-salt ore sample via chloride gravimetry.

Theoretical Foundations

Rock salt (halite) dissolves in water leaving insoluble gangue (clay, anhydrite) which is filtered off. Chloride in the filtrate is precipitated as AgCl: Ag+ + Cl- → AgCl(s), GF = 0.2473. The chloride result is converted to % NaCl using M_NaCl/M_Cl = 58.44/35.45 = 1.6487, giving the ore grade.

Required Apparatus & Chemicals

Laboratory Apparatus

  • Analytical balance
  • 400 mL beaker
  • Hot plate
  • Quantitative filter paper
  • Sintered-glass crucible
  • Oven
  • Desiccator

Chemical Reagents

  • Rock salt ore, ground
  • Nitric acid, dilute
  • Silver nitrate solution, 0.1 M
  • Distilled water

Step-by-Step Practical Procedure

  1. Weigh accurately 0.4 g of ground ore.
  2. Dissolve in 200 mL hot water; filter off insoluble gangue through quantitative paper and wash.
  3. Acidify the filtrate with HNO3 in a foil-wrapped beaker and heat.
  4. Precipitate with AgNO3, digest, filter through a weighed sintered-glass crucible.
  5. Wash, dry at 150 C to constant mass, weigh AgCl and calculate % NaCl.

Observations & Expected Results

Grey insoluble residue on the first filter; white AgCl from the filtrate. Typical AgCl mass about 0.8 g from 0.4 g ore.

Worked Stoichiometric Calculations

Problem: 0.4000 g of ore gave 0.8120 g AgCl. Calculate % Cl and % NaCl (ore grade).

Working: Mass Cl = 0.8120 × 0.2473 = 0.2008 g → % Cl = 50.20%. % NaCl = 50.20 × 1.6487 = 82.76% NaCl grade.

Safety Precautions & Hazard Control

  • Grind the ore finely for complete dissolution of halite.
  • Wash the gangue residue thoroughly; occluded brine causes low results.
  • Protect AgCl from light.

Waste Disposal Protocol

Silver residues collected for recovery.

Viva Voce Oral Defense Questions & Answers

Q: What gangue minerals occur with rock salt?

A: Clay, anhydrite (CaSO4), gypsum and sometimes potassium/magnesium salts; the insoluble ones are filtered off before precipitation.

Q: Why convert % Cl to % NaCl for ore grade?

A: The commercial product is sodium chloride, so the grade is quoted as % NaCl assuming all chloride is present as halite.