CHEMVEN

Potentiometric Determination of Iron in an Ore Sample

To determine % iron in a haematite ore by SnCl2 reduction followed by potentiometric titration with K2Cr2O7.

Level: UniversitySafety: Needs supervisionTime: 2 h
Aim of Experiment: To determine % iron in a haematite ore by SnCl2 reduction followed by potentiometric titration with K2Cr2O7.

Theoretical Foundations

Fe3+ in the dissolved ore is reduced to Fe2+ by SnCl2 (excess removed with HgCl2, giving silky Hg2Cl2 precipitate). Titration with dichromate: Cr2O7(2-) + 6 Fe2+ + 14 H+ -> 2 Cr3+ + 6 Fe3+ + 7 H2O. A Pt electrode follows the Fe3+/Fe2+ then Cr2O7(2-)/Cr3+ potentials; the dE/dV peak gives Ve. % Fe = V x M x 6 x 55.85 / sample mass.

Required Apparatus & Chemicals

Laboratory Apparatus

  • mV meter
  • Pt + reference electrodes
  • Burette
  • Digestion beakers
  • Analytical balance

Chemical Reagents

  • Haematite ore (powdered)
  • Conc. HCl (digestion)
  • SnCl2 solution
  • HgCl2 solution
  • K2Cr2O7 standard (0.02 M)
  • H3PO4 (masking)

Step-by-Step Practical Procedure

  1. Digest ~0.5 g ore in conc. HCl with heating until dissolved.
  2. Reduce Fe3+ with SnCl2 dropwise until colourless, plus 1-2 drops excess.
  3. Cool, add HgCl2 to remove excess SnCl2 (silky white precipitate).
  4. Dilute, add H3PO4 to mask Fe3+ (lowers its formal potential).
  5. Titrate potentiometrically with 0.02 M K2Cr2O7.
  6. Read Ve from the derivative peak and calculate % Fe.

Observations & Expected Results

A sharp potential jump (~300 mV) marks the endpoint; typical haematite assays 55-65% Fe.

Worked Stoichiometric Calculations

Problem: 0.5021 g ore needed 31.4 mL of 0.0200 M K2Cr2O7. Calculate % Fe.

Working: Moles Cr2O7 = 0.0314 x 0.0200 = 6.28 x 10^-4 mol; moles Fe = 6 x 6.28 x 10^-4 = 3.768 x 10^-3 mol. Mass Fe = 3.768 x 10^-3 x 55.85 = 0.2104 g. % Fe = 0.2104/0.5021 x 100 = 41.9%.

Safety Precautions & Hazard Control

  • Conc. HCl digestion: fume hood, gloves, eye protection.
  • HgCl2 is toxic; add carefully and keep the precipitate contained.
  • Standardise dichromate against pure iron wire for best accuracy.

Waste Disposal Protocol

Mercury-containing residues to mercury waste; chromium waste to Cr(VI) collection.

Viva Voce Oral Defense Questions & Answers

Q: Why is H3PO4 added before titration?

A: It complexes Fe3+, lowering the Fe3+/Fe2+ formal potential so the endpoint jump is larger and sharper, and it removes the yellow Fe3+ colour.

Q: What is the purpose of HgCl2?

A: It oxidises excess SnCl2 to Sn4+ (forming Hg2Cl2 precipitate) so the excess reductant does not consume dichromate.

Q: Why 6 Fe per dichromate?

A: Cr2O7(2-) gains 6 electrons (2 Cr(VI) -> 2 Cr(III)); each Fe2+ gives 1 electron, so 6 Fe2+ are oxidised per dichromate.

← Back to Experiments Directory